Density
|
1.54
|
g/cm³
|
ISO 1183
|
Molding Shrinkage
|
|
|
ISO 294-4
|
Across Flow
|
1.5
|
%
|
|
Flow
|
1.9
|
%
|
|
Tensile Modulus
|
406000
|
psi
|
ISO 527-2
|
Tensile Stress (Yield)
|
7690
|
psi
|
ISO 527-2
|
Tensile Strain (Yield)
|
13
|
%
|
ISO 527-2
|
Nominal Tensile Strain at Break
|
15
|
%
|
ISO 527-2
|
Tensile Creep Modulus
|
|
|
ISO 899-1
|
1 hr
|
218000
|
psi
|
|
1000 hr
|
116000
|
psi
|
|
Flexural Modulus
|
392000
|
psi
|
ISO 178
|
Charpy Notched Impact Strength
|
|
|
ISO 179/1eA
|
-22°F
|
1.9
|
ft·lb/in²
|
|
73°F
|
1.9
|
ft·lb/in²
|
|
Charpy Unnotched Impact Strength (73°F)
|
33
|
ft·lb/in²
|
ISO 179/1eU
|
Notched Izod Impact Strength (73°F)
|
1.9
|
ft·lb/in²
|
ISO 180/1A
|
Heat Deflection Temperature
|
|
|
|
66 psi, Unannealed
|
320
|
°F
|
ISO 75-2/B
|
264 psi, Unannealed
|
201
|
°F
|
ISO 75-2/A
|
Melting Temperature 3
|
352
|
°F
|
ISO 11357-3
|
CLTE
|
|
|
ISO 11359-2
|
Flow
|
5.6E-5
|
in/in/°F
|
|
Transverse
|
5.4E-5
|
in/in/°F
|
|
Flammability Classification (0.0591 in)
|
HB
|
|
IEC 60695-11-10, -20
|
Emission of Organic Compounds
|
7.50
|
µgC/g
|
VDA 277
|
|